Characteristics for grade     10KH17N13M3T   ( 10Х17Н13М3Т )



      Grade :   10KH17N13M3T   ( 10Х17Н13М3Т ) (   Х17Н13М3Т     ЭИ432   )
      Classification :   Corrosion-resistant steel for general purposes
      Equivalent grades:   Go here



Chemical composition in % for grade   10KH17N13M3T   ( 10Х17Н13М3Т )
C Si Mn Ni S P Cr Mo -
max   0.1max   0.8max   212 - 14max   0.02max   0.03516 - 183 - 4 5(С - 0.7) Ti, остальное Fe


Mechanical properties under Т=20oС for grade   10KH17N13M3T   ( 10Х17Н13М3Т )
Assortment Dimension Direct. sв sT d5 y KCU Heat treatment
- mm - MPa MPa % % kJ / m2 -
Bar, GOST 5949-75     530 196 40 55 Guenching 1050 - 1100oC,Cooling air,
Wire, GOST 18143-72     540-830  20-25   
Forging, GOST 25054-81     510 196 30-3840-50  
Sheet trick, GOST 7350-77     530 235 37   Guenching 1030 - 1080oC,Cooling air,
Sheet thin, GOST 5582-75     530   38   Guenching Cooling water,
Sheet thin, GOST 4986-79     530   20-40  Guenching 1050 - 1080oC, air,


    Brinell hardness for     10KH17N13M3T   ( 10Х17Н13М3Т )   ,     Forging GOST 25054-81 HB 10 -1 = 200   MPa


Technological properties for grade   10KH17N13M3T   ( 10Х17Н13М3Т )
  Weldability: without limitations.


Physical properties for grade   10KH17N13M3T   ( 10Х17Н13М3Т )
T E 10- 5 a 10 6 l r C R 10 9
Grade MPa 1/Grade Watt/(m·Grade) kg/m3 J/(kg·Grade) Ohm·m
20       8000    


Equivalent steels for grade     10KH17N13M3T   ( 10Х17Н13М3Т )
Warning! Indicated both exact and nearest equivalents.
USAGermanyJapanEnglandItalySpain
-DIN,WNrJIS BSUNIUNE
316Ti
S31635
1.4573
GX3CrNiMoCuN24-6-5
X10CrNiMoTi18-12
SUS316Ti
320S33
X6CrNiMoTi17-13
F.3535
X6CrNiMoTi17-12-2



Types of delivery of grade   10KH17N13M3T   ( 10Х17Н13М3Т )
B03 - Metal forming treatment. Forgings
В22 - Graded and shaped rolling
B23 - Sheets and Strips
В32 - Graded and shaped rolling
B33 - Sheets and Strips
B34 - Ribbons
В62 - Steel pipes and connecting parts to them
B73 - Steel Alloy Wire
B76 - Metal nets


Specification :
Mechanical properties :
sв - Tensile strength , [MPa]
sT - Yield stress, [MPa]
d5 - Specific elongation at fracture , [ % ]
y - Reduction of area , [ % ]
KCU - Impact strength , [ kJ / m2]
HB - Brinell hardness , [MPa]

Physical properties :
T - Test temperature , [Grade]
E - Young modulus , [MPa]
a - Coefficient of linear expansion (range 20o - T ) , [1/Grade]
l - Termal (heat) condition coefficient , [Watt/(m·Grade)]
r - Density , [kg/m3]
C - Specific heat ( range 20o - T ), [J/(kg·Grade)]
R - Electrical resistance , [Ohm·m]

Weldability :
without limitations - welding is done without heating and subsequent heat treeting
limited weldability - welding is possible under heating up to 100-120 grade and subsequent heat treeting
hard weldability - obtaining the quality welding needs the additional operations:heating up to 200-300 grade; the heat treeting ia annealing

  10KH17N13M3T   ( 10Х17Н13М3Т ) - Corrosion-resistant steel for general purposes: chemical composition, mechanical and physical properties, hardness
Database of steels and alloys (Marochnik) contains information about chemical composition and properties more then 3000 steels and alloys

    ©   2003 - 2024         Database of Steel and Alloy (russian title is the Marochnik)
Administration of the Marochnik is not responsible for the content's use.
Рейтинг@Mail.ru