Characteristics for grade     110G13L   ( 110Г13Л )



      Grade :     110G13L   ( 110Г13Л )
      Classification :   Casting alloy steel with specific properties
      Equivalent grades:   Go here



Chemical composition in % for grade   110G13L   ( 110Г13Л )
C Si Mn Ni S P Cr
0.9 - 1.50.3 - 111.5 - 15max   1max   0.05max   0.12max   1


Mechanical properties under Т=20oС for grade   110G13L   ( 110Г13Л )
Assortment Dimension Direct. sв sT d5 y KCU Heat treatment
- mm - MPa MPa % % kJ / m2 -
Casting, GOST 21357-87     800 400 25 35 Guenching 1000 - 1080oC, water,
Mechanical properties is set in consultation with the customer


Technological properties for grade   110G13L   ( 110Г13Л )
  Weldability: is not used.
 Flakes : not predisposed
Temper brittleness: not predisposed


Technological properties of the material   110G13L   ( 110Г13Л ) .
        Linear shrinkage : 2.6 - 2.7   %


Heat treatment of the material   110G13L   ( 110Г13Л )
Hardening 1050 - 1100 ° C, Water cooling


Equivalent steels for grade     110G13L   ( 110Г13Л )
Warning! Indicated both exact and nearest equivalents.
USAGermanyJapanFranceEnglandItalySpainChinaSwedenHungaryPolandRomaniaCzechiaFinlandAustriaSouth KoreaNorway
-DIN,WNrJIS AFNORBSUNIUNEGBSSMSZPNSTASCSNSFSONORMKSNS
A128
J91109
J91119
J91129
J91139
J91149
1.3401
1.3802
GX120Mn12
GX120Mn13
X120Mn12
SCMnH1
SCMnH11
SCMnH2
SCMnH3
Z120M12
Z120M12M
BW10
GX120Mn12
AM-X-120Mn12
F.240
F.8251
X120Mn12
ZGMn13-1
ZGMn13-1-4
ZGMn13-2
ZGMn13-3
2183
X120Mn13
C120G13
L120G13
T105Mn120
T130Mn135
17618
422920
G-X120Mn13
BOHLERK700
SCMnH1
1699



Types of delivery of grade   110G13L   ( 110Г13Л )
B42 - Rails: Pads, Pads, Crutches
B82 - Steel Castings
B83 - Castings with special properties (cast iron and steel)


Specification :
Mechanical properties :
sв - Tensile strength , [MPa]
sT - Yield stress, [MPa]
d5 - Specific elongation at fracture , [ % ]
y - Reduction of area , [ % ]
KCU - Impact strength , [ kJ / m2]
HB - Brinell hardness , [MPa]

Physical properties :
T - Test temperature , [Grade]
E - Young modulus , [MPa]
a - Coefficient of linear expansion (range 20o - T ) , [1/Grade]
l - Termal (heat) condition coefficient , [Watt/(m·Grade)]
r - Density , [kg/m3]
C - Specific heat ( range 20o - T ), [J/(kg·Grade)]
R - Electrical resistance , [Ohm·m]

Weldability :
without limitations - welding is done without heating and subsequent heat treeting
limited weldability - welding is possible under heating up to 100-120 grade and subsequent heat treeting
hard weldability - obtaining the quality welding needs the additional operations:heating up to 200-300 grade; the heat treeting ia annealing

  110G13L   ( 110Г13Л ) - Casting alloy steel with specific properties: chemical composition, mechanical and physical properties, hardness
Database of steels and alloys (Marochnik) contains information about chemical composition and properties more then 3000 steels and alloys

    ©   2003 - 2024         Database of Steel and Alloy (russian title is the Marochnik)
Administration of the Marochnik is not responsible for the content's use.
Рейтинг@Mail.ru