Database of Steel and Alloy (Marochnik) |
Home | Steel and Alloy | Search | Equivalent Grades | GOST Standards | Grading | Contacts |
Grade : | 14KH2GMRL ( 14Х2ГМРЛ ) |
Classification : | Casting alloy steel for general purposes |
Equivalent grades: | Is absent |
C | Si | Mn | Ni | S | P | Cr | Mo | Cu | B |
0.1 - 0.17 | 0.2 - 0.42 | 0.9 - 1.2 | max 0.3 | max 0.02 | max 0.02 | 1.4 - 1.7 | 0.45 - 0.55 | max 0.3 | max 0.004 |
Assortment | Dimension | Direct. | sв | sT | d5 | y | KCU | Heat treatment |
- | mm | - | MPa | MPa | % | % | kJ / m2 | - |
Casting, GOST 21357-87 | to 100 | 690 | 590 | 14 | 25 | 490 |
Brinell hardness for 14KH2GMRL ( 14Х2ГМРЛ ) (annealing) , | HB 10 -1 = 179 - 196 MPa |
Weldability: | hard weldability. |
Temper brittleness: | weakly predisposed |
Linear shrinkage : | 2.4 - 2.5 % |
Water hardening 920 - 930 ° C, Tempering 630 - 650 ° C |
B83 - Castings with special properties (cast iron and steel) |
Mechanical properties : | |
sв | - Tensile strength , [MPa] |
sT | - Yield stress, [MPa] |
d5 | - Specific elongation at fracture , [ % ] |
y | - Reduction of area , [ % ] |
KCU | - Impact strength , [ kJ / m2] |
HB | - Brinell hardness , [MPa] |
Physical properties : | |
T | - Test temperature , [Grade] |
E | - Young modulus , [MPa] |
a | - Coefficient of linear expansion (range 20o - T ) , [1/Grade] |
l | - Termal (heat) condition coefficient , [Watt/(m·Grade)] |
r | - Density , [kg/m3] |
C | - Specific heat ( range 20o - T ), [J/(kg·Grade)] |
R | - Electrical resistance , [Ohm·m] |
Weldability : | |
without limitations | - welding is done without heating and subsequent heat treeting |
limited weldability | - welding is possible under heating up to 100-120 grade and subsequent heat treeting |
hard weldability | - obtaining the quality welding needs the additional operations:heating up to 200-300 grade; the heat treeting ia annealing |
© 2003 - 2024 Database of Steel and Alloy (russian title is the Marochnik)
Administration of the Marochnik is not responsible for the content's use. |