Grade : | VT6S ( ВТ6С ) |
Classification : | Titanium wrought alloy |
Equivalent grades: | Go here |
Fe | C | Si | V | N | Ti | Al | Zr | O | H | Impurity |
max 0.25 | max 0.1 | max 0.15 | 3.5 - 4.5 | max 0.04 | 87.86 - 90.9 | 5.3 - 6.5 | max 0.3 | max 0.15 | max 0.015 | other 0.3 |
Assortment | Dimension | Direct. | sв | sT | d5 | y | KCU | Heat treatment |
- | mm | - | MPa | MPa | % | % | kJ / m2 | - |
Sheet, GOST 22178-76 | 835 | 10-12 | Annealing | |||||
Sheet, GOST 22178-76 | 980 | 8 | Quenching and artificial aging | |||||
Bar, GOST 26492-85 | 755-935 | 6-9 | 15-22 | 250-300 | Annealing | |||
Bar, GOST 26492-85 | 1030 | 4 | 14 | 250 | Hardening and ageing | |||
Bar, GOST 26492-85 | 755-980 | 7-10 | 22-30 | 400 | Annealing | |||
Bar, GOST 26492-85 | 1030 | 6 | 20 | 300 | Hardening and ageing |
Brinell hardness for VT6S ( ВТ6С ) (annealing) , | HB 10 -1 = 241 - 321 MPa |
Weldability: | without limitations. |
T | E 10- 5 | a 10 6 | l | r | C | R 10 9 |
Grade | MPa | 1/Grade | Watt/(m·Grade) | kg/m3 | J/(kg·Grade) | Ohm·m |
20 | 4455 |
Germany | England | ||
DIN,WNr | BS | ||
|
|
B53 - Sheets and Strips |
B55 - Bars |
Mechanical properties : | |
sв | - Tensile strength , [MPa] |
sT | - Yield stress, [MPa] |
d5 | - Specific elongation at fracture , [ % ] |
y | - Reduction of area , [ % ] |
KCU | - Impact strength , [ kJ / m2] |
HB | - Brinell hardness , [MPa] |
Physical properties : | |
T | - Test temperature , [Grade] |
E | - Young modulus , [MPa] |
a | - Coefficient of linear expansion (range 20o - T ) , [1/Grade] |
l | - Termal (heat) condition coefficient , [Watt/(m·Grade)] |
r | - Density , [kg/m3] |
C | - Specific heat ( range 20o - T ), [J/(kg·Grade)] |
R | - Electrical resistance , [Ohm·m] |
Weldability : | |
without limitations | - welding is done without heating and subsequent heat treeting |
limited weldability | - welding is possible under heating up to 100-120 grade and subsequent heat treeting |
hard weldability | - obtaining the quality welding needs the additional operations:heating up to 200-300 grade; the heat treeting ia annealing |
© 2003 - 2024 Database of Steel and Alloy (russian title is the Marochnik)
Administration of the Marochnik is not responsible for the content's use. |