Characteristics for grade     VT6   ( ВТ6 )



      Grade :     VT6   ( ВТ6 )
      Classification :   Titanium wrought alloy
      Equivalent grades:   Go here



Chemical composition in % for grade   VT6   ( ВТ6 )
Fe C Si V N TiAl Zr OH Impurity
max   0.6max   0.1max   0.13.5 - 5.3max   0.0586.45 - 90.95.3 - 6.8max   0.3max   0.2max   0.015 other 0.3
Comment: Ti is a basis; the percentage of Ti is given approximately.


Mechanical properties under Т=20oС for grade   VT6   ( ВТ6 )
Assortment Dimension Direct. sв sT d5 y KCU Heat treatment
- mm - MPa MPa % % kJ / m2 -
Sheet annealed , GOST 22178-76     885   8    
Bar, GOST 26492-85     835-1050  6-1020-30300-400Annealing
Bar, GOST 26492-85     1080   4 12200Hardening and ageing
Bar, GOST 26492-85     835-885  6-815-20250Annealing
Bar, GOST 26492-85     1080   6 20250-300Hardening and ageing
Die     950-1100  10-1335-60400-800Annealing
Plate annealed , GOST 23755-79 11 - 100   835-1080  6 12-16300 


    Brinell hardness for     VT6   ( ВТ6 )   (quenching, ageing) ,     Bar HB 10 -1 = 293 - 361   MPa
    Brinell hardness for     VT6   ( ВТ6 )   (annealing) ,     Die HB 10 -1 = 255 - 341   MPa


Technological properties for grade   VT6   ( ВТ6 )
  Weldability: without limitations.


Physical properties for grade   VT6   ( ВТ6 )
T E 10- 5 a 10 6 l r C R 10 9
Grade MPa 1/Grade Watt/(m·Grade) kg/m3 J/(kg·Grade) Ohm·m
20 1.15   8.37 4450   1600
100   8.4 9.21     1820
200   8.7 10.88   0.586 2020
300   9 11.7   0.67 2120
400   10 12.56   0.712 2140
500     13.82   0.795  
600     15.49   0.879  
T E 10- 5 a 10 6 l r C R 10 9


Equivalent steels for grade     VT6   ( ВТ6 )
Warning! Indicated both exact and nearest equivalents.
USAGermanyJapanFranceEngland
-DIN,WNrJIS AFNORBS
6Al-4V
Grade5
3.7164
3.7165
SAT-64
Ti-6Al-4V
T-A6V
Ti-P.63
Ti-Al-V



Types of delivery of grade   VT6   ( ВТ6 )
B53 - Sheets and Strips
B55 - Bars


Specification :
Mechanical properties :
sв - Tensile strength , [MPa]
sT - Yield stress, [MPa]
d5 - Specific elongation at fracture , [ % ]
y - Reduction of area , [ % ]
KCU - Impact strength , [ kJ / m2]
HB - Brinell hardness , [MPa]

Physical properties :
T - Test temperature , [Grade]
E - Young modulus , [MPa]
a - Coefficient of linear expansion (range 20o - T ) , [1/Grade]
l - Termal (heat) condition coefficient , [Watt/(m·Grade)]
r - Density , [kg/m3]
C - Specific heat ( range 20o - T ), [J/(kg·Grade)]
R - Electrical resistance , [Ohm·m]

Weldability :
without limitations - welding is done without heating and subsequent heat treeting
limited weldability - welding is possible under heating up to 100-120 grade and subsequent heat treeting
hard weldability - obtaining the quality welding needs the additional operations:heating up to 200-300 grade; the heat treeting ia annealing

  VT6   ( ВТ6 ) - Titanium wrought alloy: chemical composition, mechanical and physical properties, hardness
Database of steels and alloys (Marochnik) contains information about chemical composition and properties more then 3000 steels and alloys

    ©   2003 - 2024         Database of Steel and Alloy (russian title is the Marochnik)
Administration of the Marochnik is not responsible for the content's use.
Рейтинг@Mail.ru