Database of Steel and Alloy (Marochnik) |
Home | Steel and Alloy | Search | Equivalent Grades | GOST Standards | Grading | Contacts |
Grade : | VT3-1 ( ВТ3-1 ) |
Classification : | Titanium wrought alloy |
Equivalent grades: | Is absent |
Fe | C | Si | Cr | Mo | N | Ti | Al | Zr | O | H | Impurity |
0.2 - 0.7 | max 0.1 | 0.15 - 0.4 | 0.8 - 2 | 2 - 3 | max 0.05 | 85.95 - 91.05 | 5.5 - 7 | max 0.5 | max 0.15 | max 0.015 | other 0.3 |
Assortment | Dimension | Direct. | sв | sT | d5 | y | KCU | Heat treatment |
- | mm | - | MPa | MPa | % | % | kJ / m2 | - |
Bar, GOST 26492-85 | 930 | 6-8 | 15-20 | 250-300 | Annealing | |||
Bar, GOST 26492-85 | 930-1230 | 8-10 | 20-30 | 300 | Annealing | |||
Bar, GOST 26492-85 | 1180 | 6 | 16-20 | 180-200 | Hardening and ageing | |||
Die | 1040-1118 | 14-20 | 45-60 | 300-400 | Annealing | |||
Die | 1150-1220 | 10-12 | 32-48 | Hardening and ageing |
Brinell hardness for VT3-1 ( ВТ3-1 ) (annealing) , Die | HB 10 -1 = 269 - 363 MPa |
Brinell hardness for VT3-1 ( ВТ3-1 ) (quenching, ageing) , Die | HB 10 -1 = 302 - 415 MPa |
Weldability: | limited weldability. |
T | E 10- 5 | a 10 6 | l | r | C | R 10 9 |
Grade | MPa | 1/Grade | Watt/(m·Grade) | kg/m3 | J/(kg·Grade) | Ohm·m |
20 | 1.15 | 8.01 | 4500 | 1360 | ||
100 | 8.6 | 8.79 | ||||
200 | 9.8 | 10.04 | 0.502 | |||
300 | 10.3 | 11.3 | 0.544 | |||
400 | 10.9 | 12.92 | 0.628 | |||
500 | 11.4 | 14.24 | 0.67 | |||
600 | 15.49 | 0.712 | ||||
T | E 10- 5 | a 10 6 | l | r | C | R 10 9 |
B55 - Bars |
Mechanical properties : | |
sв | - Tensile strength , [MPa] |
sT | - Yield stress, [MPa] |
d5 | - Specific elongation at fracture , [ % ] |
y | - Reduction of area , [ % ] |
KCU | - Impact strength , [ kJ / m2] |
HB | - Brinell hardness , [MPa] |
Physical properties : | |
T | - Test temperature , [Grade] |
E | - Young modulus , [MPa] |
a | - Coefficient of linear expansion (range 20o - T ) , [1/Grade] |
l | - Termal (heat) condition coefficient , [Watt/(m·Grade)] |
r | - Density , [kg/m3] |
C | - Specific heat ( range 20o - T ), [J/(kg·Grade)] |
R | - Electrical resistance , [Ohm·m] |
Weldability : | |
without limitations | - welding is done without heating and subsequent heat treeting |
limited weldability | - welding is possible under heating up to 100-120 grade and subsequent heat treeting |
hard weldability | - obtaining the quality welding needs the additional operations:heating up to 200-300 grade; the heat treeting ia annealing |
© 2003 - 2024 Database of Steel and Alloy (russian title is the Marochnik)